Carbide Grade 牌号 | WC Grain Size 晶粒尺寸 | Binder 粘合剂 | Binder Content%w/w 粘合剂含量 | Density g/㎝3 密度 | Hardness HV30 硬度 | Hardness HRA 硬度 | Transverse Rupture StrenghN/㎜2 抗弯强度 | Pressure Resistance* N/㎜2 抗压强度 | Fracture Toughness** N/㎜2.m1/2 断裂韧性 | Special Properties 特性 |
RX8UF | Ultrafine 超细 | Cobalt 钴 | 8 | 14.52 | 1880 | 93.6 | 3800 | 6300 | 8.5 | |
RX12UF | 12 | 14.06 | 1680 | 92.6 | 4200 | 6000 | 9.5 | |||
RX3 | Submicron 亚微米 | Cobalt 钴 | 3.3 | 15.15 | 2000 | 94.2 | 3000 | 6500 | 7.8 | |
RX6 | 6 | 14.83 | 1820 | 93.3 | 3300 | 6400 | 8.5 | |||
RX7 | 7.5 | 14.65 | 1740 | 92.9 | 3500 | 6300 | 9.0 | |||
RX10 | 10 | 14.43 | 1600 | 92.1 | 3700 | 6000 | 9.8 | |||
RX15 | 15 | 13.95 | 1370 | 90.4 | 4000 | 5500 | 12.5 | |||
RF13 | Fine 细 | Cobalt 钴 | 6.5 | 14.83 | 1690 | 92.7 | 2600 | 5700 | 9.2 | |
RF24 | 12 | 14.28 | 1380 | 90.5 | 3000 | 4800 | 11.2 | |||
RF40 | 20 | 13.52 | 1080 | 87.2 | 3500 | 4000 | 18 | |||
RF54 | 27 | 12.94 | 890 | 84.7 | 3600 | 3600 | >20 | |||
RM13 | Medium 中 | Cobalt 钴 | 6.5 | 14.83 | 1580 | 92.0 | 2700 | 5500 | 9.5 | |
RM16 | 8.5 | 14.64 | 1500 | 91.4 | 2800 | 5300 | 10.4 | |||
RM22 | 11 | 14.41 | 1390 | 90.5 | 2900 | 5000 | 11.8 | |||
RM30 | 15 | 14.01 | 1230 | 88.9 | 3200 | 4500 | 14.5 | |||
RCR17 | Medium 中 | Cobalt 钴 | 8.5 | 14.5 | 1600 | 92.1 | 2900 | 5400 | 10.0 | EDM grades with corrosion inhibitor EDM牌号,耐电腐蚀 |
RCR24 | 12 | 14.15 | 1400 | 90.6 | 3200 | 5000 | 13.0 | |||
RCR30 | 15 | 13.85 | 1200 | 88.5 | 3400 | 4500 | 17.5 | |||
RB14 | Coarse 粗 | Cobalt 钴 | 7 | 14.81 | 1450 | 91.0 | 2800 | 4800 | 10.0 | Coarse grain material of high toughness 粗颗粒,高韧性 |
RB10 | 10 | 14.48 | 1300 | 89.7 | 3000 | 4400 | 12.5 | |||
RB15-H | 15 | 14.03 | 1080 | 87.2 | 3100 | 3800 | 18.5 | |||
RB20-H | 22 | 13.44 | 870 | 84.5 | 3200 | 3300 | >20 | |||
RCS12 | Submicron 亚微米 | Nickel 镍 | 6 | 14.8 | 1700 | 92.7 | 2600 | 5400 | 8.1 | Corrosion-resistant (nonmagnetic) 耐腐蚀,无磁 |
RCS17 | 8.5 | 14.5 | 1650 | 92.4 | 2800 | 5200 | 8.5 | |||
RCS24 | 12 | 14.09 | 1370 | 90.4 | 3000 | 4800 | 10.2 | |||
RCN | Fine 细 | Nickel镍 | 8 | 14.53 | 1600 | 92.1 | 2600 | 5100 | 8.3 | |
RCFN22 | Nickel/Chromium | 11 | 14.33 | 1600 | 92.1 | 1800 | 4500 | 8.0 | ||
RCM30 | Medium 中 | Nickel 镍 | 15 | 14.00 | 1100 | 87.3 | 2900 | 4000 | 13.0 | Corrosion-resistant 耐腐蚀 |
RXE20 | Submicron 亚微米 | Iron/Nickel/Cobalt 铁/镍/钴 | 10 | 14.10 | 1600 | 92.1 | 3200 | 5500 | 10.8 | high toughness 高韧性 |
RXE40 | 20 | 13.05 | 1250 | 89.1 | 3600 | 4000 | 18.5x |
Standard ISO codes define grain sizes from fine to medium and do not represent the today’s state of the art in cemented carbides. The selection of the optimum carbide grade should therefore always be done based on application data of the customer.
标准 ISO 代码定义粒度由细至中等,并没有反应最先进的硬质合金发展成果。最佳的硬质合金牌号的选择应因此始终基于客户的实际应用的数据。
ISO | K10 | K20 | K30 | K40 | K10-F | K20-F | K30-F | G10 | G20 | G30 | G40 |
ESTECH GRADE | RF13 | RM13 | RM16 | RM22,RF24 | RX6 | RX7 | RX10 | RM16 | RM22,RF24 | RM30 | RF40 |